PETG settings for the Anycubic Kobra S1

OrcaSlicer's Anycubic PETG profile prints at 250 °C, with the bed at 70 °C and the part fan at 30 to 90 %.

Profile Nozzle Bed Part fan Max flow Retraction
Anycubic PETG 250 °C 70 °C 30 to 90 % 12 mm³/s 1.5 mm
AliZ PETG 250 °C 79 °C 30 to 80 % 15 mm³/s 0.8 mm
AliZ PETG-Metal 260 °C 79 °C 30 to 80 % 13 mm³/s 0.8 mm
Bambu PETG Basic 255 °C 70 °C 10 to 40 % 13 mm³/s 0.8 mm
Bambu PETG HF 245 °C 70 °C 20 to 40 % 12 mm³/s 0.8 mm
Bambu PETG Translucent 245 °C 70 °C 10 to 30 % 6 mm³/s 0.3 mm
COEX PETG 245 °C 80 °C 30 to 50 % 16 mm³/s 4 mm
Elas PETG Basic 250 °C 80 °C 20 to 100 % 13 mm³/s 0.8 mm
OrcaSlicer has 35 more PETG profiles for this printer.

How do I set up my file for the Anycubic Kobra S1?

Drop it here. It opens in Convert with the Anycubic Kobra S1 and Anycubic PETG picked, and nothing converts until you click Convert.

Which build plate should I use?

Anycubic PETG sets a bed temperature for each plate:

  • Textured PEI plate: 70 °C
  • Smooth PEI plate: 70 °C
  • Cool plate: 55 °C
  • Engineering plate: not supported

Why is my PETG stringing?

Lower the nozzle toward 220 °C, the floor Anycubic PETG declares, and lengthen retraction (Prusa Knowledge Base). Wet PETG strings more, and Bambu Lab dries it at 60 to 65 °C for 8 hours in a forced-air oven (Bambu Lab wiki).

Why does PETG print so slowly?

Anycubic PETG caps flow at 12 mm³/s, and the slicer slows any move that would push more plastic than that (slicer source).

Why won't my PETG stick?

Anycubic PETG heats the bed to 70 °C, so if a part still lifts, clean the sheet first (Prusa Knowledge Base). On smooth PEI, apply a glue stick first, since PETG can bond hard enough to damage the sheet (Prusa Knowledge Base).

Where do these values come from?

From the profiles OrcaSlicer ships, read at OrcaSlicer v2.4.2 (8500fcd). Where a filament profile leaves retraction unset, the table shows the printer profile's value.